Peel strength Pipe surface temperature, (23±2)° C Use a knife cut width 10mm,length greater than 100mm Pipe Wrapping Tape layer until pipe body .Then use spring balance with a 90degree direction to pull ,speed not more than 300mm/min,peel strength should get no less than 25N/cm. The test should be done 24 hours after tape wrapping .
Qiangke Factory Peel Strength Test on Pipe Wrapping Tape with 0.5mmThickness.
Objective: To evaluate the peel strength of 980-20 inner tape.
Specification: 0.5mm
March 1, 2025 Qiangke factory on the production of 980-20 polyethylene anti corrosion tape peel strength test.
Test method:
Standardï¼ASTM D1000
Test Video Please visit:https://studio.youtube.com/video/TalOU8o3oLA/edit
Peel strength
Pipe surface temperature, (23±2)° C
Use a knife cut width 10mm,length greater than 100mm Pipe Wrapping Tape layer until pipe body .Then use spring balance with a 90degree direction to pull ,speed not more than 300mm/min,peel strength should get no less than 25N/cm.
The test should be done 24 hours after tape wrapping .
Date:
Peel Adhesion to Primed Steel
1ã30N/cm
2ã27 N/cm
3ã29 N/cm
4ã29 N/cm
5ã28 N/cm
Conclusion: Qualified